Two thick-film resistors cracked across their short axes during thermal cycling after vibration tests. Analyses pointed to bending failure and several possible stress factors but did not establish a single root cause
At hot-dwell temperatures, two resistors on identical printed circuit boards intermittently opened electrically, then recovered at room temperature. Each was a large 2512-size thick-film ceramic chip resistor, and each fracture ran across the component's short axis in a single straight line. The failures appeared during thermal cycling after vibration testing.
What The Analyses Found
NASA's National Engineering Safety Center (NESC) reported that both resistors were near the edges of their boards and came from the same production lot. Independent failure analyses found no clear crack-initiation site. Optical and scanning electron microscopy found no clear signs of fatigue damage; the transverse cracks were consistent with bending or tensile loading rather than twisting or cyclic vibration fatigue.
The shared production lot prompted concern about defective parts. The lot met procurement specification MIL-PRF-55342, and additional testing found no direct evidence of a lot defect. NESC's conclusion was that no direct root cause had been identified; the findings focused attention on mechanical loads imposed by the board assembly.
Stress At The Board Edge
The NESC identified several possible contributors rather than a confirmed root cause: the resistors were positioned near board edges with their long axes parallel to those edges; solder extended onto the tops of the terminations; and board bow or twist could create bending loads. Rigid mounting and fastener-torquing patterns could also concentrate stress at the component locations. In surface-mount assemblies, local strain is affected by board thickness, support points, component location and orientation.
Board flexure can load a ceramic component as the board bends. Excess solder on top of a termination can make the joint more rigid and transfer movement into the resistor body. NASA's work also includes volunteer-led research, as covered in its 2026 citizen science awards; this bulletin addresses the separate problem of hardware reliability.
Assembly Precautions
The NESC bulletin advises placing large ceramic components so their long axes do not run parallel to nearby board edges. When edge placement is necessary, it recommends finite element analysis to assess stress and displacement margins. Assemblers should keep solder off the tops of terminations and follow manufacturer limits for fillet height.
The recommendations also include inspecting physical joints or photographs of them, using controlled mounting and fastener practices, and performing one to three thermal cycles with a functional hot-dwell test before vibration testing. The bulletin cites MIL-STD-202 Method 218, Board Flex, as a reference.
In this failure mode, board flexure means bending or twisting of the circuit board that transfers mechanical load to a mounted component. A rigid ceramic resistor can crack under that load, while solder on top of its termination can make the connection less able to accommodate movement. The two failures were detected during environmental acceptance testing, but the NESC did not identify a single root cause.